Electroplating nickel of alumium
From Efficiency Finder
Revision as of 12:41, 18 November 2010 by Breka (Talk | contribs) (Protected "Electroplating nickel of alumium" [edit=autoconfirmed:move=autoconfirmed])
Back to EFFICIENCY FINDER FOR METAL INDUSTRY
- Typical parameters of the process
Process | Temperature [°C] | Chemicals | Concentration [g/l] | Details | Literature |
"Kanigan" process for nickel plating on aluminium | 93-96 | 1. Nickelsulfate(NiSO4 7H2O), 2. Sodiumhypophosphite (NaH2Po2 H2O), 3. Complexing agents and puffers, 4. Accelerator, 5. Stabilizer, 6. Surfacant | 1. 19-26 g/l, 2. 23-30 g/l, 3. 30-50 g/l. 4. 2-4 g/l, 5. 2-4 mg/l, 6. 30-50 mg/l | pH: 4,3- 4,7, precipitation speed: 25-28 μm/h | Oberflächenbehandlung von Aluminium; T.W. Jelinek, Eugen G. Leue Verlag, D- 88348; 1997 |